| Physico-mechanical indexes of complex polyamide yarn |
| № | Index name | Norm for yarn |
| Complex | Monofilament |
| Sort B | Sort А | Sort B | Sort А |
| 3,3; 6,7; 5 tex | 15,6 tex | 1,67; 2,2 tex | 2,2 tex | 3,3 tex |
| Highest quality | 1st quality | Highest quality | 1st quality | Highest quality | 1st quality | Highest quality | 1st quality | Highest quality | 1st quality |
| 1. | Specific (relative) tearing force, cN/tex, not less | 39,2 | 39,2 | 37,3 | 36,3 | 44,1 | 44,1 | 44,1 | 41,2 | 44,1 | 41,2 |
| 2. | Relative lengthening at break, % | 31,0±3,0 | 36,0±5,0 | 29,0±3,0 | 37,0±4,0 | 40,0±5,0 |
| 3. | Coefficient of variation at lengthening, %, not more | 13,0 | 14,0 | 15,0 | 15,0 | 13,0 | 14,0 | 16,0 | 18,0 | 16,0 | 19,0 |
| 4. | Relative deviation of conditioned linear density from nominal one, % | ±2,5 | ±2,5 | ±3,5 | ±2,5 | ±2,5 | ±3,0 | ±2,5 | ±3,0 |
| 5. | Coefficient of variation at linear density measured on specific yarn parts with the length 1 m, %, not more | 2,5 | 3,0 | - | - | 3,0 | 3,5 | 3,0 | 3,5 | 3,5 | 3,8 |
| 100 m of curls, %, not more | - | - | 3,0 | 3,5 | - | - | - | - | - | - |
| Twists number per 1 m of yarn | 200±10 300±20 | 100±15 | - | - | - | - | - | - |
| 6. | Winding density, g/cm3 for 1,67 tex | 0,74±0,10 - | 0,74±0,10 - | 0,74±0,10 0,60±0,10 | 0,74±0,10 - | 0,74±0,10 - |
| 7. | Mass share of spin finish, %: in bobbins in cops |
3,0±1,0 - |
2,0±1,0 - |
2,0±1,0 - |
2,0±1,0 1,2±0,8 |
2,0±1,0 1,5±1,0 |
| 8. | Linear shrinkage of yarn, % | not more 7,0 | 14,5±1,5 | not more 7,0 | 14,5±1,0 | 15,0±2,0 |
| 9. | Mass share of low-molecular substances(LMS), %, not more for yarn, produced on home spinning machines | - | - | - | - | - | - | - | - | 3,8 |
|
|