Physico-mechanical indexes to polyamide (PА-6) cord caprone fabrics. ГОСТ 24221-94 (TU U 17.2-00204048.147-2001) |
| № | Index name | Norm for fabric |
| 6 KNTS-0 | 123KNTS | 23KNTS | 232KNTS | 25KNTS | 252KNTS | 28KNTS | 282KNTS |
| 1. | Cord yarn structure | 93,5 tex х1 | 93,5 tex х1х2 | 187 tex х1х2 | 187 tex х1х2 | 187 tex х1х2 | 187 tex х1х2 | 187 tex х1х2 | 187 tex х1х2 |
| 2. | Thickness, mm | 0,3±0,03 | 0,5±0,03 | 0,7±0,03 | 0,7±0,03 | 0,7±0,03 | 0,7±0,03 | 0,7±0,03 | 0,7±0,03 |
| 3. | Tearing force, N, not less | 57 | 122 | 225 | 225 | 245 | 245 | 275 | 275 |
| 4. | Coefficient of variation at tearing force, %, not more | 8,0 | 3,8 | 3,8 | 3,8 | 3,8 | 3,8 | 3,8 | 3,8 |
| 5. | Yarn lengthening, %, at force 20 N |
| 8,0±1,5 | 4,5±1,5 | 4,5±1,5 | 4,5±1,5 | 4,5±1,5 | 4,5±1,5 | 4,5±1,5 |
| 6. | Yarn lengthening, %, at force 39 N |
| 12,0±1,5 | 8,5±1,5 | 8,5±1,5 | 8,5±1,5 | 8,5±1,5 | 8,5±1,5 | 8,5±1,5 |
| 7. | Yarn lengthening, %, at break | 20,0±3,0 | 27,0±2,0 | 27,0±2,0 | 27,0±2,0 | 28,0±2,0 | 28,0±2,0 | 28,0±2,0 | 28,0±2,0 |
| 8. | Coefficient of variation at lengthening at break, %, not more |
| 7,0 | 7,0 | 7,0 | 7,0 | 7,0 | 7,0 | 7,0 |
| 9. | Thermal stability, %, not less |
| 80 | 80 | 80 | 80 | 80 | 80 | 80 |
| 10. | Linear shrinkage, %, not more |
| 11,0 | 11,0 | 11,0 | 11,0 | 11,0 | 11,0 | 11,0 |
| 11. | Mass share of spin finish, %, not more | 1,2 | 1,2 | 1,2 | 1,2 | 1,2 | 1,2 | 1,2 |
|
| 12. | Twists number per 1 m, I twisting | 300±20 | 470±20 | 336±20 | 336±20 | 336±20 | 336±20 | 336±20 | 336±20 |
| 13. | Twists number per 1 m, II twisting |
| 470±20 | 328±20 | 328±20 | 328±20 | 328±20 | 328±20 | 328±20 |
| 14. | Twisting direction | Z | ZZS | ZZS | ZZS | ZZS | ZZS | ZZS | ZZS |
| 15. | Fabric width, cm | 148±2 | 148±2 | 148±2 | 148±2 | 148±2 | 148±2 | 148±2 | 148±2 |
| 16. | Filaments number per 10 cm on warp | 94±1 | 61±1 | 94±1 | 75±1 | 94±1 | 75±1 | 94±1 | 75±1 |
| 17. | Filaments number per 10 cm on weft | 12±1 | 10±1 | 8±1 | 10±1 | 8±1 | 10±1 | 8±1 | 10±1 |
| 18. | Bindness strength of cord yarn with rubber, N, not less | 785 |
|
|
|
|
|
|
|
| 19. | Surface density, g/m2 | 95±20 | 132±10 | 406±20 | 325±15 | 406±20 | 325±15 | 406±20 | 325±15 |
| 20. | Mass share of low-molecular combinations, %, not more | 3,0 |
|
|
|
|
|
|
|
| 21. | As a weft a cotton yarn 25 tex is used |
| 22. | First two figures mean tearing force in N; the third figure-difference in densities of warp and weft; К-caprone fabric |
| 23. | N-cord fabric produced out of cord yarn without water treatment; Т-fabric thermal treated; S-fabric out of stabilised caprone cord yarns; О-cord fabric produced on the base of monotwisted yarn |
|
|